Summary
A plasterer gets the call a week after finishing: "it's cracked." The customer sees a network of hairline cracks like crazy paving across a wall, or a straight crack every 1.2 m, or a crack above the door, and wants to know whether the plaster has to come off. Nearly always it does not. Crazing is a surface fault in the top millimetre, caused by the finish coat losing its water faster than it could set, and the cure is cosmetic. Straight cracks at regular spacing are the board joints telegraphing through, because the tape was missed or the joints were not filled before the skim, and the cure is local. A crack that follows a line of weakness in the wall, or that opens further every month, is the building moving and the plaster is the messenger.
Separating the three takes a torch held flat to the wall, a straightedge, a note of where the cracks are and a conversation about what the room has been doing for the last fortnight (heating, dehumidifier, open windows, new boards, old lath). This guide gives the diagnosis by crack pattern, the causes in order of how often they happen, the fixes for each with time and cost, and the application rules that stop it recurring. For skim technique see skim coat; for drying see plaster drying times by type; for board jointing see scrim tape and jointing.
Key Facts
- Crazing (map cracking) — a fine, interconnected network of hairline cracks, usually across a whole area, in the top 1–2 mm of a gypsum finish; the surface shrank as it dried faster than the body of the coat set. Cosmetic. Does not flake unless the bond has also failed
- Suction — the rate the background draws water out of wet plaster. High-suction backgrounds (dry bonding coat, browning, old plaster, aerated blocks, bare plasterboard paper in hot weather) must be controlled with a PVA bonding agent or a proprietary primer, or wetted down, before skimming. Uncontrolled suction is the first cause of crazing
- Drying conditions — gypsum skim should dry naturally at 10–20°C with background ventilation; heating on full, a dehumidifier, direct sun through a window or a fan heater pointed at a wall pulls the water out before the set. The second cause of crazing
- Over-trowelling and late trowelling — polishing the surface too long, or trowelling after the plaster has started to go off, brings fat (fine gypsum and water) to the surface which shrinks and crazes; adding water to re-wet a set surface does the same
- Coat thickness — finish plaster at 2 mm per coat and 3–5 mm total; a single thin coat crazes, a thick coat over 5 mm cracks and can slump. Bonding coat 8–11 mm per coat, browning or hardwall up to 11 mm
- Skimming over a wet basecoat — a bonding or hardwall coat skimmed before it has set and had its initial dry (usually 24 hours minimum) shrinks under the skim and cracks it in random lines
- Plasterboard joints — every joint must be scrimmed (self-adhesive fibreglass scrim 50 mm, or paper tape bedded in jointing compound) and the joint filled before the skim; a missed joint shows as a straight crack along the board edge within weeks. Cut edges and board ends are the usual misses
- Board fixing — boards fixed at over 300 mm centres, or with the screws missing the stud, flex and crack the joints; screws at 300 mm maximum on walls, 230 mm on ceilings, 12 mm from the board edge
- Dot and dab — dabs at too wide a spacing, or boards not pressed back to a continuous line of dabs at the perimeter and around openings, flex at the joints
- Corners and openings — cracks running diagonally from the corners of doors and windows are the classic sign of board or lintel movement; a straight crack at an internal corner where two walls meet is differential movement between a stud wall and a masonry wall, or a missed internal-corner scrim
- Old cracks — a skim over an old crack in a masonry wall re-opens along the same line unless the crack was raked out, filled, and bridged with scrim or a fibre mesh; sound-sounding old plaster that is hollow behind will crack and drum
- Lath and plaster — skimming over old lime plaster on timber lath: the lath moves with humidity and the new gypsum does not; cracks follow the lath lines. Bond with a flexible primer or overboard
- Lime vs gypsum — lime plaster shrinks as it carbonates and crazes if dried too fast or applied too thick; the fix is the same (fill or re-work), but the materials are not interchangeable; see lime plaster
- Structural cracks — over 5 mm wide, stepped through brickwork, tapering, or growing: BRE Digest 251 categorises crack widths from 0 (hairline, under 0.1 mm) to 5 (over 25 mm); category 2 and above (over 1 mm) merits investigation. Not a plastering fault
- Thermal and shrinkage cracks in new build — new timber-frame and new masonry shrink for 12–18 months; fine cracks at the ceiling-to-wall junction and at board joints are expected in year one and are filled at the end of the defects period. NHBC Standards allow this
- Time on site — fill and sand crazing on one wall 1–2 hours plus drying; rake out, scrim and re-skim one joint 1 hour plus drying; re-skim a crazed wall 2–3 hours
Quick Reference Table
Diagnosed the problem? Create a repair quote in minutes with squote.
Try squote free →| Pattern | Where | Most likely cause | Fix |
|---|---|---|---|
| Fine map-like network over a whole area | Any skim | Suction uncontrolled, or dried too fast | Fill with fine filler or re-skim over primer |
| Fine network only where sun or a heater reached | One wall or part | Dried too fast locally | As above; control drying next time |
| Straight cracks at 1.2 m or 0.9 m spacing | Plasterboard walls and ceilings | Joints not scrimmed or filled | Rake out, scrim, fill, re-skim locally |
| Straight crack along a board end or cut edge | Walls at the ends of runs | Cut edge not scrimmed; board end unsupported | Scrim and re-skim; add a noggin if the end flexes |
| Random lines, slightly raised, in the skim | Over a basecoat | Basecoat skimmed before it set | Rake out and fill; if widespread, strip and re-do |
| Diagonal crack from a door or window corner | Above openings | Board or lintel movement; no scrim across the corner | Scrim diagonally across the corner, re-skim; check lintel if it grows |
| Crack at the internal corner of two walls | Where stud meets masonry | Differential movement; no corner scrim | Flexible filler or scrim and re-skim; accept a hairline in new build |
| Crack following an old crack line | Re-skimmed masonry | Old crack not raked and bridged | Rake out, fill, mesh, re-skim |
| Lines following lath spacing | Old lath and plaster | Lath movement under gypsum | Overboard or bond with flexible primer and re-skim |
| Wide, stepped, tapering or growing crack | Anywhere | Structural movement | Monitor; refer to a surveyor; do not fill yet |
Detailed Guidance
Diagnostic sequence
NEW PLASTER HAS CRACKED
│
├─ Hold a torch flat to the surface. What does the crack pattern look like?
│ │
│ ├─ FINE NETWORK (map / crazy paving), hairline, over an area
│ │ └─ CRAZING. Ask: was the background primed? Heating/dehumidifier on?
│ │ Sun on the wall? Trowelled late or re-wetted?
│ │ ──► Cosmetic: fill or re-skim over a controlled background
│ │
│ ├─ STRAIGHT LINES at regular spacing (board widths) or along board ends
│ │ └─ JOINTS. Tap: hollow? Flex the board: does the crack open?
│ │ ──► Rake out, scrim, fill, re-skim locally; fix board fixings first
│ │
│ ├─ RANDOM RAISED LINES in a skim over a basecoat
│ │ └─ BASECOAT SHRINKAGE: skimmed too soon
│ │ ──► Rake and fill; strip and re-do if widespread
│ │
│ ├─ DIAGONAL from opening corners / straight at an internal corner
│ │ └─ MOVEMENT at a weak point. Hairline and stable?
│ │ ├─ Yes ──► scrim across and re-skim; flexible filler at corners
│ │ └─ Growing ──► check lintel / structure
│ │
│ └─ WIDE (over 1 mm), stepped, tapering, growing, or through the masonry
│ └─ STRUCTURAL. Measure, photograph, date. Refer. Do not plaster over.
│
└─ Does the plaster sound hollow or flake at the crack?
└─ BOND FAILURE as well: strip the loose area back to sound, prime, re-plaster
Crazing: the surface dried before it set
Gypsum finish plaster sets by crystallisation, which needs the mixing water to stay in the coat for the first 20–40 minutes. If the background draws the water out (suction), or the air takes it (heat, draught, sun, dehumidifier), the surface shrinks before it has set and splits into the fine map pattern. It is almost always the top millimetre. Run a fingernail across it: if the surface is hard and the cracks do not catch, it is crazing and the plaster underneath is sound.
The usual causes, in order: skimming a dry bonding coat, browning, old plaster or sand-and-cement without a PVA or primer coat (or with the PVA fully dried and skimmed hours later rather than while tacky); skimming plasterboard in hot weather without a mist of water or a primer; the customer putting the heating on full and shutting the windows the moment the plasterer left; direct sun on one wall through a south-facing window; and over-trowelling or re-wetting a surface that had started to go off, which draws fat to the surface. Ask the customer what the room did in the first 48 hours. The answer usually ends the argument about whose fault it is.
The fix is cosmetic. For light crazing, two coats of a fine surface filler applied with a wide blade and sanded, then a mist coat and the finish paint, hides it. For heavy crazing, or where the customer will see it under a sheen paint, prime the wall with a bonding agent as the manufacturer directs and re-skim with a single tight 2 mm coat, then let it dry naturally for a week before painting. Do not re-skim over unprimed crazed plaster; the suction that crazed the first coat will craze the second.
Straight cracks: the joints are showing
Cracks at 1.2 m or 900 mm spacing on a wall, or in a grid on a ceiling, are plasterboard joints. Every joint, including cut edges and board ends, must be reinforced with scrim or paper tape and filled flush before the skim; a joint that was scrimmed but not filled can also show, because the skim is thin over the scrim and thick either side. Tap along the crack: a hollow sound means the board is not fixed back to the stud or the dabs there, and the joint is flexing. Press the board; if the crack opens, the fixing is the fault.
Fix the fixing first: add screws at 300 mm centres into the studs either side of the joint (230 mm on ceilings), or, on dot and dab, inject a foam adhesive behind a hollow board through a 10 mm hole. Then rake the crack out to a V with a scraper, brush out the dust, bed a 50 mm scrim or a paper tape in jointing compound, fill flush, and re-skim a band 150 mm either side feathered into the existing plaster. On a ceiling, where the board ends run across the joists, a crack along an unsupported board end needs a noggin added between the joists before it is scrimmed. See plasterboard fixing and dot and dab and scrim tape and jointing.
Cracks over a basecoat skimmed too soon
A bonding coat or a hardwall skimmed while it was still soft, or the same day in cold damp conditions, shrinks under the finish and cracks it in random lines, sometimes with the skim lifting slightly along the crack. The basecoat should have set hard and had its initial drying (24 hours minimum, longer in cold weather) before it is keyed and skimmed; a basecoat that is still dark and cold to the touch is not ready. If the cracking is local, rake it out, fill with the finish plaster and re-skim the patch. If it is across a whole wall, the honest repair is to strip the skim and the loose basecoat back to the background and start again, because the shrinkage will continue under a patch. See bonding coat application.
Corners, openings and old cracks
Diagonal cracks from the top corners of doors and windows are the commonest crack in any house because the board or the masonry is weakest there, and the lintel and the frame move differently from the wall. In a new skim they appear within weeks. Rake out, bed a scrim diagonally across the corner (a 300 mm strip at 45°) and re-skim. If the crack re-opens and grows wider than a hairline, the lintel is moving and the plaster is not the problem; see lintel replacement.
An internal corner where a stud partition meets a masonry wall will always have a hairline, because the two move differently. A flexible decorator's caulk in the corner before painting is the standard answer; scrim and skim will crack again. A crack in a re-skimmed masonry wall that follows exactly the line of an old crack was never bridged: rake it out to 10 mm wide and deep, fill with a bonding or a crack-repair compound, bed a fibre mesh over it 100 mm either side, and re-skim. Hollow old plaster around the crack will also need to come off; it is better found now than when the paint lifts. See patch repairs.
When it is not the plaster
Any crack over 1 mm wide, any crack that steps through the brick or block joints outside, any crack that is wider at one end than the other, and any crack that has grown between two visits a month apart is movement in the building, and the plaster is simply the first thing to show it. Measure the width with a crack gauge, photograph it with a date, fix a tell-tale or a pencil mark across it, and come back in four to six weeks. BRE Digest 251 puts hairline-to-1 mm cracks in categories 0 and 1 (aesthetic, filled at redecoration) and 1–5 mm in category 2 (fill, may need some re-pointing or small repairs); above 5 mm, or growing, is category 3 and upward and needs a structural engineer or a surveyor before anyone plasters over it. Tell the customer in writing; a plasterer who fills a structural crack and takes the blame when it re-opens has bought someone else's problem. See structural engineer survey and render crack diagnosis for the outside of the same wall.
New-build shrinkage
In a new house or a new extension, timber studs, joists and the blockwork dry out and shrink for 12–18 months, and hairline cracks appear at the ceiling-to-wall junction, at board joints and at the corners of openings. NHBC Standards and most warranty providers treat these as normal and expect them to be filled at the end of the first year, not re-plastered. Explain this before the customer calls it a defect, and offer the end-of-year fill as a priced visit.
Fixes, time and cost
| Repair | Time | Typical charge (2026) |
|---|---|---|
| Fill and sand light crazing, one wall, ready for mist coat | 1–2 h | £80–£150 |
| Prime and re-skim one crazed wall (12–15 m²) | 2–3 h | £150–£260 |
| Rake out, scrim and re-skim one joint crack, including re-fixing | 1 h | £70–£120 |
| Rake, mesh and re-skim an old crack line, 2 m | 1–1.5 h | £90–£160 |
| Scrim and re-skim both corners of an opening | 1 h | £80–£140 |
| Strip and re-do a wall where the basecoat was skimmed too soon | Half to one day | £250–£450 |
| Overboard a cracked lath-and-plaster ceiling and skim (12 m²) | 1 day | £450–£750 |
Where the fault is the original plasterer's and within a reasonable period, the Consumer Rights Act 2015 entitles the customer to a repeat performance at no cost; where the fault is the customer's drying regime, say so politely and charge. Either way, put the drying instructions on the invoice next time: no heating above 20°C, no dehumidifier, windows on trickle vent, and no paint for a week.
Frequently Asked Questions
Does crazed plaster need to come off?
No, unless it also sounds hollow or flakes at the cracks. Crazing is in the surface, and the plaster beneath has set and bonded. Fill it, or prime and re-skim it. Only plaster that has lost its bond to the background (hollow, drumming, lifting) needs to come off back to sound material.
The customer put the heating on and now it's cracked. Whose fault is it?
Drying too fast is the customer's doing if they were told not to and did; it is the plasterer's if they were not told. The surface crazing is cosmetic either way and the repair is a filler and a sand, so the cheapest answer is usually to do it and to put the drying instructions in writing on every job from now on. A plasterer who leaves a written drying note on the wall has the argument won before it starts.
Can I just paint over hairline cracks in new plaster?
Over crazing, a fine filler and two coats of a good matt emulsion hides most of it; a flexible paint or a lining paper hides the rest. Over a joint crack or a corner crack, paint will crack along the same line within a month because the board is still moving; scrim and re-skim it first. Over a crack that is growing, nothing should go on until the cause is known.
Why has my new skim cracked in straight lines when the old wall never did?
Because the old wall was probably lath and plaster or a solid-plastered masonry wall, and the new skim is over plasterboard, which has joints every 1.2 m. The joints are the weak line, and if any were left without scrim, or the boards are not fixed at every stud, they will show. It is a board-jointing fault, not a plaster fault, and it is fixed joint by joint.
How long should new plaster be left before painting?
Until it has dried to an even pale pink (gypsum) or pale grey (sand and cement) with no dark patches: 3–7 days for a skim over board in a warm, ventilated room, longer over a wet basecoat or in winter, and 4 weeks or more for sand and cement. Then a mist coat of watered-down emulsion before the finish coats. Painting over dark, damp plaster traps the water and causes blistering and flaking, and painting over crazing without filling shows every crack through the sheen. See plaster drying times by type.
Regulations & Standards
BS EN 13279-1:2008 — gypsum binders and gypsum plasters; definitions and requirements
BS EN 13279-2:2014 — gypsum binders and gypsum plasters; test methods
BS EN 13914-2:2016 — design, preparation and application of external rendering and internal plastering; internal plastering
BS 8212:1995 — code of practice for dry lining and partitioning using gypsum plasterboard
BS EN 520:2004+A1:2009 — gypsum plasterboards; definitions, requirements and test methods
BS 8000-10:1995 — workmanship on building sites; code of practice for plastering and rendering
BS EN 998-1:2016 — specification for mortar for masonry; rendering and plastering mortar
BRE Digest 251 — assessment of damage in low-rise buildings; crack width categories 0–5
NHBC Standards, Chapter 8.2 — wall and ceiling finishes; tolerances and expected shrinkage cracking in new homes
Consumer Rights Act 2015, s.49 and s.55 — services performed with reasonable care and skill; right to repeat performance
British Gypsum — The White Book, plastering guidance — suction control, coat thickness, drying and board jointing requirements
BRE Digest 251: Assessment of damage in low-rise buildings — BRE — crack classification and when to investigate
NHBC Standards — wall and ceiling finishes — tolerances and shrinkage cracking in new build
BS 8212 dry lining code of practice — BSI — plasterboard fixing and jointing
Finishing plaster technical datasheets — Gyproc / Saint-Gobain — application thickness and setting times
skim coat — applying a finish coat correctly
plaster drying times by type — when it is dry enough to paint
scrim tape and jointing — reinforcing board joints
plasterboard fixing and dot and dab — fixing boards so they do not flex
patch repairs — repairing cracks and hollow plaster
render crack diagnosis — the same wall from outside